With the large-scale continuous casting equipment, the unit steel flow rate in the ladle shroud has gradually increased, from less than 1t/min to more than 7t/min at present. The increase in the steel flow rate per unit time has caused a sharp scouring of the inner wall. Therefore, the scouring of the inner wall has become the determining factor of the service life of the large-scale shroud. Table 1 shows the corresponding relationship between the steel flow rate per unit time and the cause of damage of large-scale shrouds at home and abroad.
| Steel Plant | Unit steel throughput (tons/minute) | Lifespan (furnace) | Total steel production (tons) | Main causes of damage |
| Domestic 1 | 4.5 | 10 | 1800 | Perforation below the neck, erosion of the slag line |
| Foreign 1 | 4.6 | 5 | 1750 | Perforation below the neck |
| Domestic 2 | 6 | 10 | 1800 | Blocks falling off at the slag line, perforation below the neck |
| Foreign 2 | 6.6 | 4 | 1200 | Perforation below the neck, transverse neck |
| Foreign 3 | 7.5 | 3 | 900 | Perforation below the neck |
Ways to improve the service life of ladle shroud
Some scholars have studied the general relationship of one-to-one without other complex factors that change the relationship, and pointed out that there is a proportional or inverse relationship between various performance indicators of refractory materials. If you want to improve one of the properties, you have to reduce other properties at the same time. The relationship between porosity and thermal shock resistance is an example. When the porosity increases, there are more vacancies in the microstructure to prevent crack propagation, so the thermal shock resistance improves. When the porosity decreases, the thermal shock resistance decreases (i.e., a proportional relationship). Table 2 shows the relationship between the various properties of the material.
| Table 2 Relationship between various properties of refractory materials | ||||||
| Material properties | Porosity | Volume density | Intensity | Wear resistance | Thermal state | Thermal shock resistance |
| Porosity | Inversely proportional | Inversely proportional | Inversely proportional | Inversely proportional | ||
| Volume density | Inverse ratio | Directly proportional | Directly proportional | Directly proportional | Inverse ratio | |
| Strength | Inverse ratio | Directly proportional | Directly proportional | Directly proportional | Inverse ratio | |
| Thermal state | Inverse ratio | Directly proportional | Directly proportional | Inversely proportional | Inverse ratio | |
| Thermal shock resistance | Direct ratio | Inversely proportional | Inversely proportional | Inversely proportional | Inversely proportional | |
| Chemical corrosion | Direct ratio | Inversely proportional | Inversely proportional | Wear resistance | Inversely proportional | One |
01 Optimization of carbon content in ladle shroud
In order to improve the thermal shock stability of ladle shroud, a high content of graphite is generally added. However, graphite carbon has low strength and is easily washed away by high-speed steel liquid, which reduces the life of ladle shroud. Therefore, optimizing the carbon content of shroud and taking into account the material’s washability and thermal shock stability is a feasible approach. A long-life aluminum carbon shroud has been developed to achieve long life by reducing carbon content and increasing the bonding strength of the binder.
02 Optimization of particle size composition
The optimization of particle size composition plays an important role in the design of shroud formula. The particle stacking theory generally includes the close stacking of discontinuous size particles and the close stacking of continuous size particles. Some people have proposed the theory of close stacking of discontinuous size particles. They believe that when small particles just fill the gaps between large particles, the most dense stacking is formed. Then the expression of multi-grade discontinuous size stacking is expressed by equation, as shown in formula (1). CPFT⁄100=(γlogD−γlogDs)⁄(γlogDl−γlogDs)(1)
In formula (1), CPFT is the cumulative percentage of raw material mass below a certain particle size, γ is the ratio of the mass of particles in two adjacent particle sizes, D is the particle size, Ds is the particle size of the smallest particle, and Dl is the particle size of the largest particle.
Andreassen proposed the theory of close packing of particles of continuous size. He believed that the distribution form of particles is the same, that is, statistically similar, and the same is true for the increase of particles. This theory is expressed by an equation, as shown in formula (2).
CDFT⁄100=(D⁄Dl)q(2)
In formula (2), q is a value, which represents the particle size distribution coefficient. Comparing the above two formulas, there is no minimum particle size limit in equation (2), and the minimum particle size can be infinitely small. The idea of finite minimum particle size is introduced to correct the Andreassen equation, as shown in formula (3).

The maximum packing density can be obtained by using discontinuous particles, but there are particle segregation and uneconomical in actual production. It is undoubtedly a better method to select continuous particles with reasonable grading and adjust the proportion of each particle size to achieve a high packing density. When the particle grading meets the most compact packing, the volume density of the formed material is the highest. Therefore, we adjust the particle grading of the material so that the material’s porosity, volume density, flexural and compressive strength and other performance indicators reach the required range, and obtain excellent thermal shock resistance and good erosion resistance.
Research results show that in order to ensure that the continuous casting “three major parts” have high thermal shock stability, a large amount of flake graphite (>20%) is usually added. The larger the particle size ratio, the worse the uniformity of the material will be, and the easier it will be to form a graphite zone. At the same time, the risk of cracks at the contact interface between coarse particles and graphite is greater, thereby reducing the thermal shock stability of the sample. However, when the amount of fine powder is too large, the thermal shock stability of the sample will also become poor due to low strength and easy crack expansion. In terms of improving thermal shock resistance, the optimal particle size composition is a ratio of 40/60 between aggregate and fine powder.
03 Select the appropriate amount of binder
The appropriate amount of binder can obtain the appropriate porosity and strength index. The study selected resin as a binder and used a high-speed granulator to granulate when the ratio of aggregate, fine powder, micropowder and graphite remained unchanged. The effect of resin addition on the granulation effect was studied through screening analysis of the prepared mud, SEM morphology observation of the sample and time-to-time analysis of physical performance indicators. The results show that with the increase of resin addition, the diameter and number of pseudo-particles formed in the mud increase, and the apparent porosity and volume density of the sample are mainly affected by the granulation effect, and then gradually change to be affected by the amount of resin added. The room temperature compressive strength and flexural strength of the sample show a trend of gradual increase.
04 Introduce low thermal expansion coefficient materials
A preheating-free long nozzle was developed by adding fused quartz and zirconium mullite, with a service life of 4 to 7 hours. On the basis of studying foreign technology, we use high-grade refractory raw materials such as Sialon and special binders, and experimentally develop production and firing processes that are compatible with the formulation technology to solve the contradiction between the thermal stability of the shroud and the erosion resistance and corrosion resistance, and obtain good comprehensive performance of the baking-free shroud products. In order to improve the thermal shock stability, low expansion refractory raw materials are generally added to the aluminum carbon shroud, such as fused quartz, zirconium mullite, silicon carbide, etc.