There are four main reasons for the damage of ladle porous plug bricks: thermal stress, mechanical wear, mechanical stress and chemical erosion. The external effects on porous plug bricks during use are shown in Figure 1.

Thermal stress effect
In actual production, the ladle temperature reaches more than 1000℃, and the molten steel temperature reaches more than 1600℃. The temperature difference between the two when in contact will produce large thermal stress, which in turn causes a very large thermal shock. The ladle is in a repetitive working environment. The thermal stress caused by the frequent temperature changes of the porous plug brick when it contacts the molten steel and the ladle is one of the reasons for the damage of the porous plug brick. The key factor for the thermal stress of the air brick is the change of temperature, and the temperature changes of different parts of the air brick are different.
The difference between the thermal stress generated by the internal parts of the porous plug brick and the temperature change at the same position is compared. It is found that the thermal stress near the working surface exceeds the bonding strength of the brick itself to a certain extent. The porous plug brick is subjected to a strong thermal shock, resulting in layered peeling of the working surface of the brick, which leads to the destruction of the air brick.
The temperature field formed at the bottom of the ladle when the molten steel enters and exits the ladle and the stress field generated by the molten steel are numerically simulated and analyzed, and numerical detection is performed. Research has found that if the ladle is to reach a “quasi-steady state”, the preheated ladle needs to be thermally cycled several times. Since the stress of the working layer near the ladle wall at the bottom of the ladle is higher than that near the center, in order to reduce the thermal stress generated there, an insulation device can be added near the ladle wall to alleviate this phenomenon.

Mechanical wear effect
The scouring of the porous plug brick by turbulence can be roughly divided into three situations:
1. When the porous plug brick is higher than the seat brick, the main reason for the damage of the brick is that the molten steel in the ladle forms a vortex that produces a huge shear effect and scouring effect on the side of the porous plug brick. Therefore, the scouring force is one of the reasons why the base bricks of the air-permeable bricks are greatly damaged. In a normal working environment, the air-permeable base bricks are used only once. After one time, the structure above the base bricks will be washed away;
2. When the air-permeable bricks are level with the base bricks, the base bricks protect the air-permeable bricks from erosion and damage. The vortex formed by the molten steel first scours the base bricks, causing the shear force of the air-permeable bricks to decrease accordingly;
3. When the air-permeable bricks are lower than the base bricks, cold steel is easy to accumulate on the working surface during normal work. Since the viscosity of the remaining cold steel is relatively large, it has a certain obstruction to the blowing, so the blowing pressure needs to be increased to meet the refining requirements. In this way, the scouring force of the air flow on the air-permeable bricks is correspondingly increased, and the shear and impact strength are large, making them more easily damaged. In order to meet the requirements of the blow-through rate and service life of the refining outside the furnace, the air-permeable bricks must have excellent anti-scouring ability and high-temperature mechanical properties.
When there are differences in refining conditions, the aggregate and matrix are appropriately proportioned to reduce the effects of erosion and penetration on the blow-through rate and service life of the air-permeable bricks.
Mechanical stress effect
During use, the working surface of the bricks at the bottom of the ladle is in direct contact with the high-temperature molten steel. Under the condition of cyclic use, the temperature in the ladle is always in a state of change. For example, the temperature difference will occur when the refractory material at the bottom of the ladle changes from high temperature to low temperature during use. Since the expansion coefficient of the original layer of the refractory material is different from that of the metamorphic layer, the bricks are subjected to shear stress, resulting in transverse cracks in the brick structure and even fracture.
Chemical erosion effect
The working layer of the porous plug brick is in contact with the steel slag and molten steel for a long time, and the slag continuously erodes and penetrates into the air bricks. Oxides such as MnO, MgO, SiO2, FeO, and Fe2O3 in molten steel and slag react with the refractory materials in the air bricks:
12CaO+7Al₂O₃=12CaO·7Al₂O₃
FeO+Al₂O₃=FeO·Al₂O₃
2MnO+SiO₂+Al₂O₃=2(MnO)·SiO₂·Al₂O₃
Physical erosion caused by melting and peeling of the working layer of the porous plug brick by molten steel, and chemical erosion caused by continuous penetration of slag and molten steel into the porous plug brick during the smelting process are the main causes of damage to the bricks. Therefore, in order to improve the thermal shock resistance and slag resistance of the material, it is necessary to improve the toughness and permeability of theporous plug brick.