The sliding gate plate is a key material for steel casting operations. During use, it must withstand high temperature, thermal shock, erosion and erosion of molten steel, and repeated opening and closing, etc. The ladle sliding gate used by a well-known domestic steel plant is a two-layer structure, as shown in Figure 1. Based on field use experience, the damage factors during the use of the slide are divided into three categories: thermal shock damage, thermochemical erosion and improper operation.

1 Thermal shock damage-sliding gate plate
The temperature of the sliding gate plate is very low before use, and during the pouring process, the slide gate plate comes into contact with high-temperature molten steel in a short time. The huge temperature difference generated will have a strong thermal shock effect on the slide gate plate body. At this time, tensile stress is generated outside the slide gate plate pouring hole. Once this stress exceeds the strength of the slide gate plate material, radial microcracks will form. Such cracks are conducive to the diffusion, aggregation, and penetration of foreign molten steel, slag, and oxygen, and become a cause of aggravated chemical corrosion.
2 Thermochemical erosion
When the slide gate plate comes into contact with high-temperature molten steel and slag during use, a series of chemical reactions will occur, causing thermochemical erosion. This type of erosion can easily cause the high-temperature wear resistance of the sliding gate plate working surface to deteriorate, the surface layer to fall off, resulting in poor fit of the slide gate plate, increased gaps, and further air intake, further oxidation erosion, and the above processes will alternate, which may cause serious accidents such as sliding gate plate leakage. During the use of the sliding gate plate, according to the different steel types and slag compositions, common thermochemical erosion phenomena can be divided into the following categories.
2.1 Chemical erosion of Ca-treated steel-sliding gate plate
In the process of producing aluminum-killed steel and silicon-aluminum-killed steel, in order to improve the castability of molten steel, Ca-Al wire and Ca-Si wire are fed into the molten steel in the refining stage for Ca treatment. When producing such steel grades, the erosion part of the slide plate presents an obvious “horseshoe” shape. The main reason is that [Ca] and CaO in the molten steel react with Al2O3 and SiO2 in the slide plate to form low-melting point compounds. Especially when the slide plate is in the pouring state, the molten steel flows in the sliding gate plate hole and easily forms a negative pressure zone. Under the action of the negative pressure zone, Ca vapor directly reacts with the inhaled oxygen to form CaO, and is enriched in this area, resulting in “horseshoe” shaped corrosion.
2.2 Chemical erosion of high Mn steel
When pouring high Mn steel grades such as pipeline steel, the slide plate expands more seriously, and the maximum expansion can reach 5mm·furnace-1; in addition, the erosion of the contact surface of the slide plate is also more serious, accompanied by the phenomenon of surface contact surface peeling and crack aggravation. This is because the MnO in the high manganese steel liquid reacts with the Al2O3 and SiO2 in the slide plate in the following chemical reactions:
MnO+SiO2MnO·SiO2, MnO+Al2O3→MnO·Al2O3,
which causes the main corrosion and thermal shock resistant materials of the slide plate, corundum and zirconium mullite, to decompose, thereby aggravating the erosion of the steel liquid and causing the aperture to expand abnormally.
2.3 Chemical erosion of slag
In the later stage of ladle pouring, due to the suction effect of molten steel flow, part of the slag will be drawn into the ladle nozzle, causing slag erosion on the slide. Its main characteristics are hole expansion and plate surface erosion, and there is also the phenomenon of crack aggravation. The composition of slag is relatively complex, mainly including CaO, SiO2, Al2O3, MgO, MnO, FeO, Cr2O3, CaF2, etc. Among them, most of the oxides can form low-melting point compounds with Al2O3 and SiO2 in the slide. In addition, FeO, MnO, etc. may also react with the carbon raw materials in the slide, causing decarburization, making the surface structure of the slide loose and causing damage.
3 Operational factors
Through practical summary, the operational factors that cause damage to the slide can be summarized into three categories: slide installation, pouring flow control and ladle nozzle oxygen burning.
(1) Unreasonable slide installation. When the slide plate is not strictly leveled when installed in the sliding mechanism, it warps or the slide plate is clamped loosely, which will generate a lot of external stress during use, leading to the overall damage of the slide plate.
(2) Unreasonable pouring flow control during production. If the flow control operation is unreasonable during the pouring process, it is easy to cause peeling, erosion, steel clamping and other phenomena on the working surface of the slide plate. Summarizing the flow control operation in production, it is found that the main reason for the damage of the slide plate is that the slide plate movement amplitude is too large or the movement is too frequent. In particular, the number of slide plate damages caused by manual flow control is more than that caused by computer automatic flow control, indicating that human factors in operation are also an important cause of slide plate damage.
(3) Unreasonable oxygen burning operation. When the ladle is prepared or there is no downflow during the pouring process, oxygen must be burned on the ladle nozzle. Once the oxygen burning operation is improper, serious oxygen burning erosion will occur. Improper oxygen burning operations that cause damage to the slide include: blowing oxygen when the slide is not completely aligned, causing oxygen to directly impact the working surface of the slide; blowing oxygen when the drainage sand has not completely flowed out, it is difficult to boil, resulting in a long oxygen blowing time; the oxygen pipe is not parallel to the flow channel, causing the oxygen flow to scour the side walls of the slide hole, forming an expanded hole, etc. In addition, other improper operating factors include unreasonable ladle turnover time, resulting in a drop in the overall temperature of the ladle, and a large thermal shock when it is used again; improper ratio of fire clay for the slide, uneven stirring, impurities, etc.
The above-mentioned damage mechanisms interact and promote each other during the preparation and use of the slide, and it is difficult to attribute the damage of the slide to a single reason. Therefore, in order to improve the service life of the slide, a comprehensive analysis must be conducted and a systematic solution must be proposed.