Magnesium carbon brick mixing

Mixing is a very important task in production. The quality of mud mixing directly affects the final quality of the product. It not only tests the carefulness of the staff, but also tests the staff’s proficiency in operation and the degree of judgment of mud. mixing process Theoretically, the mixing order and feeding method should be as follows:

First add coarse particles and medium particles, stir for a period of time, then add resin, stir for a period of time, then add graphite, stir for a period of time, and finally add fine powder and various additives, and then stir evenly.

Although the quality of the mixed mud has a certain relationship with the mixer, there is no absolute relationship, which mainly depends on human operation. The key point lies in the judgment of the situation in the mixer. Different formulas, different batches of binders (phenolic resins), different manufacturers, and the temperature in the mixer and the total category of the mixer may lead to different time control at each stage of mixing.

But in the end, the same effect must be achieved: the graphite tightly wraps the aggregate particles, the clay temperature is moderate, warm but not hot, the clay is uniform in thickness, there is no segregation, the clay feels soft and not prickly when held tightly, and the clay clumps when released, but it can naturally disperse when thrown back into the hopper.

However, such an effect is often not achieved in actual operation. For example, the particle size is not accurate, resulting in a large particle size. When it exceeds a certain range, it will feel prickly when holding the clay tightly with your hand. If the particle size is small and exceeds a certain range, it will feel soft; for example, the quality of many phenolic resins is not stable enough due to the profit-seeking reasons of merchants. If the volatility of the resin is not clear, it is easy to mix the clay with moisture or dryness when mixing. In addition, when the mixed clay is sent to the machine for molding, it is found that the remaining clay is completely dry after half of it is used, and production cannot be carried out.mixing process

Experience and data in the production process

(1) Check the accuracy of the raw material particle size classification. If the size of the particle size material itself is not accurately controlled, the material prepared according to the formula will definitely be inaccurate. For example, if 5~3mm particle size material is added at 25%, but 30% of the raw material smaller than 3mm has been mixed into the 5~3mm particle size material, the amount of 5~3mm particle size material added will definitely be insufficient, so the particle size classification of the raw material must be accurate.

(2) Check whether the fine powder raw material is agglomerated. The smaller the particle size of the raw material, the easier it is to absorb moisture. Therefore, many fine powder raw materials are basically produced on the spot, especially magnesium sand fine powder is easy to absorb moisture and agglomerate.

(3) Check the volatility of the resin. Generally, the test method is used to check. Phenolic resin is generally purchased in batches, and the performance of each batch of resin is relatively stable unless there is an abnormality in the production process. When each batch of resin enters the factory, do not put it into production directly. Instead, take a small amount of experimental mixing 1-2 times to see the effect, to judge the quality of the resin, and then determine whether the resin can be used. Of course, you can also sample the resin for testing, but in actual production, the laboratory test data can only be used as a reference, and the final result still depends on the experimental mixing results. Check the resin temperature. In summer, the resin temperature should be controlled between 20~30℃, and in winter, it should be controlled between 25~40℃. If the resin temperature is too low, it will affect the fluidity of the resin. When mixing, the resin cannot be dispersed, which will easily lead to the appearance of resin balls in the mud. If the temperature is too high, it will easily cause the resin to deteriorate.

(4) Determine the ambient temperature and the temperature of the mixer, and control the working mode and mixing time of the mixer according to the temperature. The temperature has a great influence on the preparation of the mud. Spring and autumn are more suitable for production. The temperature in summer is too high, the resin evaporates quickly, and the mud dries quickly, so the temperature should not be too high, especially for high-speed mixers. The water cooling system must be turned on. The temperature is low in winter, especially in southern Liaoning, which is the main production area of ​​magnesia carbon bricks. The temperature here is basically around minus 10 degrees Celsius, so remember to turn on the heating system of the mixer. The 750 mixer is basically unusable in winter unless the insulation measures of the factory are very good; the rotary multifunctional and efficient mixer must turn on the heating system, because the temperature in winter is too low, and the heat generated by its friction is not enough to ensure the temperature of the mud; the high-speed mixer is turned on as appropriate according to the actual ambient temperature, because the heat generated by the friction of the high-speed mixer is very large, and the temperature of the mud can be guaranteed when the ambient temperature is not too low. If the ambient temperature is too low, it must be turned on.mixing process

Mixing method in actual production

Mixer model: high-speed mixer

First add granular material (5-3, 3-1, 1-0) → mix at low speed for 1~3 minutes → then add resin → mix at low speed for 1~2 minutes → then add graphite → mix at low speed for 1~2 minutes → finally add fine powder and premix → mix at low speed for 1 minute → high-speed net mixing time (carbon content ≤10% high-speed mixing for 10-12 minutes; carbon content>10% high-speed mixing for 12~15 minutes);

Mixer model: rotary high-efficiency mixer

First add granular material (5-3, 3-1 , 1-0) → low speed mixing for 1~3 minutes → then add resin → low speed mixing for 1~2 minutes → → then add graphite à low speed mixing for 1~2 minutes → finally add fine powder and premix → low speed mixing for 1 minute → medium speed net mixing time for 25~35 minutes;

Mixer model: 750 mixer

First add granular material (5-3, 3-1, 1-0) → low speed mixing for 3~5 minutes → then add resin → low speed mixing for 2~3 minutes → then add graphite → low speed mixing for 2~3 minutes → finally add fine powder and premix → low speed mixing for 45~50 minutes.

When mixing, pay attention to the following points

(1) If it is winter, after the granular material is added, the low speed mixing time should be appropriately extended, especially in the morning after taking over, because the temperature of the mixer is low, it is necessary to stir at a low speed for a while to increase the temperature of the mixer. If it is summer, it is just the opposite, and the mixing time should be appropriately reduced.

(2) When workers mix materials, in addition to following the mixing regulations, they must also check the state of the clay in real time and check the feel of the clay regularly to confirm whether the clay is qualified, under-mixed or over-mixed.

(3) In order to avoid mixing errors that lead to continued errors in the next process, a regular spot check system must be strictly implemented. It is very important to formulate a reasonable spot check system, but this is the job of the quality manager. Mixers must pay attention to sampling, retaining samples and sending samples according to standards.mixing process

How do fluctuations in resin temperature during the mixing process affect the performance in steel plants?

Resin temperature directly determines the uniformity of the slurry. If the temperature is too high in summer, the resin is prone to deterioration or rapid volatilization, leading to a decrease in the bonding strength of the bricks. If the temperature is too low in winter (below 20℃), the resin has poor fluidity and is prone to forming “resin balls,” resulting in micropores or segregation inside the bricks. For steel plants, this directly manifests as a decrease in the anti-stripping performance of magnesia-carbon bricks at high temperatures, shortening the service life of the furnace lining or ladle.

Why must magnesia-carbon brick production follow the sequence of “coarse to fine, staged feeding”?

A: The scientific sequence (coarse/medium particles → resin → graphite → fine powder/additives) ensures that graphite is tightly coated on the surface of the aggregate particles. If the feeding sequence is disordered, it will lead to uneven graphite distribution or additive ineffectiveness. For steel plants, a uniform microstructure provides better resistance to slag penetration, preventing steel slag from eroding the interior through the brick gaps, thereby maintaining the stability of the furnace lining structure.

How can the physical properties of finished magnesia-carbon bricks be predicted by observing the state of the clay?

Qualified clay should be in a state where it “can be formed into a ball when squeezed in the hand, crumbles when dropped, is not prickly to the touch, and is not hot.”
Prickly to the touch: This indicates inaccurate particle grading, with too many coarse particles, making the finished bricks prone to cracking.
Hot: This indicates excessive mixing time or excessive frictional heat generation, leading to pre-curing of the resin, resulting in bricks with high hardness but poor toughness.
When accepting products, steel mills can request suppliers to provide records of the mixing process parameters as an important reference for product consistency checks.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.
Contact Information