lmm@magnesiacarbonbricklmm.com

Technical support and construction service team

What are the methods and precautions for adding drainage sand?

As a key material in the ladle sliding nozzle system, the addition method and precautions of drainage sand directly affect the automatic pouring rate of the ladle, the quality of molten steel and production safety. The following is a detailed analysis from the two aspects of addition method and precautions:

drainage sand

1. Method of adding drainage sand

1. Manual throwing method: After the hot repair of the ladle is completed, the whole bag of drainage sand is thrown from the top of the ladle to the water inlet manually, and the drainage sand falls into the water inlet by gravity.

Features: The equipment is simple and the cost is low, but the throwing accuracy is poor, which can easily lead to uneven accumulation of drainage sand or insufficient filling. The packaging bag is easy to mix with drainage sand, which affects the fluidity, and the labor intensity is high, which poses a safety hazard.

Application scenario: It is suitable for small-scale production or temporary emergency scenarios, and has been gradually eliminated in large steel mills.

2. Duct weight sand adding method: The drainage sand is poured into the water inlet from the top of the ladle through a long duct, and the flow rate and filling amount are controlled by the counterweight device.

Features: It can reduce manual intervention, and the filling position is relatively accurate, but the drainage sand in the duct is prone to particle size segregation (coarse particles sink and fine particles float), resulting in uneven sintering layer thickness. The counterweight device needs to be maintained regularly to avoid affecting the filling accuracy due to wear.

Application scenario: It is suitable for ordinary steel grades with low requirements for self-opening rate.

3. Mechanical funnel sand adding method: Use a special sand adding bucket to accurately deliver the drainage sand to the water inlet through the cantilever device, and the amount of sand added and the shape of the accumulation can be controlled.

Features: high degree of automation, accurate amount of sand added (error ±5%), regular accumulation shape (mushroom-shaped), which is conducive to the formation of a uniform sintering layer.

It can reduce the waste of drainage sand (consumption is reduced by 10-15%), but the equipment maintenance cost is high.

Application scenario: widely used in continuous casting production lines, especially for medium and high alloy steel grades.

4. Automatic sand adding method: Use industrial robots, visual positioning systems and servo control devices to realize automatic grabbing, bag breaking, filling and quality inspection of drainage sand.

Features: fully automated operation, positioning accuracy of ±2mm, high filling efficiency (single furnace sand adding time ≤2min). The amount of sand added and the accumulation status can be monitored in real time, the self-opening rate is increased to more than 99%, and dust pollution is reduced.

Application scenario: suitable for high-end steel grades (such as bearing steel, electrical steel) and large-scale automated production.

5. Backflow sand adding method: reverse pouring drainage sand from the bottom of the ladle to avoid residue blocking the water inlet when adding sand at the top.

Features: It can prevent the residue on the top of the ladle from falling into the water inlet, improve the filling quality, and is suitable for ladles with more residue. The equipment is complex and requires a bottom sealing device, and the application range is limited.

Application scenario: ladle maintenance under special working conditions.

2. Precautions for adding drainage sand

1. Preparation before adding

Water inlet cleaning: Use an oxygen gun to thoroughly clean the residual steel and residue in the water inlet and the seat brick to ensure that the inner wall is smooth, and avoid the residue and drainage sand reacting to form high melting point substances (such as FeO and SiO₂ to form iron olivine, melting point 1100℃), resulting in too thick sintering layer.

Drainage sand drying: Dry at 100-200℃ for 2-4 hours before use to remove moisture (water content ≤0.2%). Excessive moisture will cause steam expansion at high temperature, making the drainage sand structure loose, and the steel liquid will penetrate to form steel sand aggregate, reducing the self-opening rate.

2. Addition process control

Particle size gradation: The particle size of conventional chromium drainage sand is controlled at 0.1-2mm, of which 1-2mm particles account for 70%, ensuring the bulk density (3.0-3.2g/cm³) and fluidity (repose angle ≤30°). 10-15% alumina particles can be added to the drainage sand for high manganese and high aluminum steel to inhibit the promotion of Mn and Al on sintering.

Addition amount: According to the size of the nozzle, the addition amount of the standard ladle (150-200t) is 40-60kg, ensuring that the filling height exceeds the upper surface of the nozzle seat brick by 50-60mm, forming a “mushroom-shaped” accumulation to prevent the steel liquid from directly scouring the nozzle wall.

Ambient temperature: Add sand when the ladle temperature is ≥800℃ to avoid the decrease in the fluidity of the drainage sand due to low temperature. If the ladle temperature is insufficient, the nozzle can be baked to above 500℃ in advance.

3. Quality inspection after adding

Stacking state: Visually check whether the drainage sand is full and without depression. If segregation (local coarse particle accumulation) occurs, it needs to be refilled.

Sintering performance test: Sampling is carried out for high-temperature sintering test (1550℃ insulation for 2h), requiring the apparent porosity ≤5%, radial shrinkage ≤5%, ensuring that the sintered layer is dense and has moderate strength (compressive strength 1-3MPa), which can prevent the penetration of molten steel and can be broken by the static pressure of molten steel.

4. Targeted measures for special steel grades

High manganese and high aluminum steel: Use alumina-chromite mixed drainage sand (Al₂O₃ content ≥20%), and use the low reactivity of Al₂O₃ with Mn and A in molten steel to reduce the generation of liquid phase. Rapid steel tapping after adding sand, shorten the exposure time of drainage sand, and avoid long-term high-temperature sintering.

Clean steel: Use zirconium drainage sands (ZrO₂ content ≥ 60%), which has poor wettability with molten steel (contact angle > 90°), reduce inclusion contamination, and control the sintering layer thickness ≤ 1mm.

The addition method of drainage sand needs to be combined with the characteristics of steel type and production scale. The core is to ensure uniform filling and controllable sintering. The future development trend is fully automated sand addition and intelligent monitoring. Sensors are used to monitor the temperature and sintering status of drainage sand in real time to further improve the self-opening rate and molten steel quality.

LMM YOTAI established in 2007. Our production technology comes from Japanese Yotai. As an experienced and international player in the refractories industry. We have succeeded in expanding both the breadth of its product range and the depth of its services. From raw material selection, refractory portofio & optimization, installation & services & recycle of used refractories on site to further reduce client’s Opex & Capex in refractory consumption per ton steel output, meanwhile improve product quality of client.

Our Product have been supplied to world’s top steel manufacturer Arcelormittal, TATA Steel, EZZ steel etc. We do OEM for Concast and Danieli for a long time

Facebook
LinkedIn
Pinterest
Reddit

Comprehensive solution of Refractory for steelmaking

Fill out the form below, and we will be in touch shortly.