The slag line is the part of the ladle where molten steel is in direct contact with air. Due to the temperature difference and oxygen-rich environment, the erosion rate in this area is significantly faster than in other parts. Furthermore, the tilting of molten steel and slag removal during operation cause considerable damage to the slag line. Therefore, the erosion of the slag line has always been a bottleneck problem in the steelmaking and ironmaking industries. The slag line not only experiences rapid erosion but also problems such as slagging, red-hot discoloration, spalling, and steel leakage. Slag line bricks generally refer to the refractory bricks laid in the area from the third to the eighth layer downwards from the ladle opening.
Currently, in steelmaking production, magnesia-carbon refractory materials are widely used in the slag line area. From the earlier magnesia-carbon brick laying to the later monolithic casting of magnesia-carbon castables, considering the lining problems in the refining process, the slag line area is still the most severely affected and has the most serious damage impact on the overall furnace lining life. Today, we will discuss this issue through multiple case studies, focusing on damage to the slag line, refractory material analysis, smelting conditions, and raw materials.
Equipment and Operating Conditions of Ladle Refining Furnaces
Common ladle refining furnaces include LF furnaces, VD furnaces, VOD furnaces, RH furnaces, and AHF furnaces. Common refractory material problems at the slag line in ladles include rapid slag line erosion, reddening of the refractory lining, the appearance of holes, slag grooves, or deep pits at the slag line. Erosion is most common and severe at the slag line of LF furnaces.
The operating conditions for refining steel ladles are as follows:
1) LF refining temperature: 1550~1610℃, refining time: 35-45min;
2) VD furnace vacuum degassing, treatment temperature: 1550~1610℃, time: greater than 20min;
3) White slag is produced during refining, using refining synthetic slag and submerged arc slag, with high basicity (CaO to SiO2 mass ratio greater than 3.5);
4) Bottom-blown argon stirring throughout the process;
5) The average tapping temperature is above 1650℃, and the average residence time of molten steel in the ladle is above 130min.With the development of secondary refining technology for steel ladles, refractory materials for steel ladles are also constantly evolving. They must possess the following characteristics: resistance to high temperatures, thermal shock, and slag erosion; high mechanical strength; and the ability to withstand continuous agitation and scouring with the molten steel.
Erosion of Slag Line Sections in Ladles
The main causes of erosion in slag line sections can be summarized into four aspects: First, process factors, including stirring intensity, power supply, and processing time during steelmaking; second, the composition of the refining slag, specifically the influence of elements such as F, MgO, Al2O3, CaO, and TFe on the slag line bricks; third, the quality of refractory materials and masonry; and fourth, mechanical damage.
Among these factors, refining slag causes the greatest damage to magnesia-carbon bricks. Different steel grades and impurities result in varying degrees of damage to the slag line bricks. The erosion process generally follows this pattern: oxidation → decarburization → loosening → erosion → detachment → destruction.
Oxidation of ladle slag line bricks is primarily carbon oxidation, including gas-phase oxidation, liquid-phase oxidation, indirect oxidation, and the influence of porosity.
Gas-phase oxidation refers to the direct oxidation of carbon, occurring when graphite coexists with air (O2), water vapor (H2O), and carbon dioxide at high temperatures.
Liquid-phase oxidation refers to the oxidation of carbon caused by iron and manganese oxides in the slag. Typically, during smelting, the rate of damage to magnesia-carbon lining bricks increases with the total iron content in the slag. In this process, as a decarburized layer forms on the surface of carbon-containing products, the slag easily penetrates and reacts, leading to a porous lining brick structure and accelerating product damage.
Indirect oxidation occurs at high temperatures when MgO reacts with carbon to form a decarburized layer, resulting in a deterioration of the magnesia-carbon brick’s microstructure. This process is the most severe, as the slag continuously erodes the decarburized layer, forming a reaction layer with magnesia sand, producing low-melting-point substances, ultimately causing melting and erosion of the magnesia-carbon brick.
Slag buildup at the ladle slag line refers to a portion of molten steel remaining at the slag line after pouring. The main reasons for this are:
Firstly, the long waiting time before pouring allows slag to form and solidify at the slag line.
Secondly, when the aluminum content in the steel slag is high, the molten steel has a high viscosity and solidifies at the slag line area of the ladle as the slag surface temperature decreases during the slag calming process.Thirdly, the slag line bricks in the ladle themselves are subject to erosion, resulting in pits or depressions (during the slag pouring process, as the alkalinity in the steel slag changes, the lining bricks in contact with the slag on the ladle wall are gradually dissolved and detached, forming these depressions). Once the alkalinity in the molten slag stabilizes, the molten slag and slag line bricks dissolve and combine to form a new slag layer, with increasing slag formation and easier slag adhesion.
How to improve the damage to the slag line?
This is a question that many scholars and steelmaking workers have been researching. Based on case studies from multiple steel plants and laboratory verifications, we propose the following points for reference:
1. Optimize the refining system and improve smelting conditions. During the refining process, lightly calcined dolomite is often added to increase the concentration of magnesium oxide in the slag, thereby increasing the basicity and viscosity of the slag and reducing the FeO content. Experiments by multiple manufacturers have shown that controlling the FeO content in the slag to around 0.5% and the MgO content to around 12%, along with adjusting the slag viscosity, can effectively reduce the erosion of magnesia-carbon bricks by the slag.
2. Use better refractory materials. The erosion resistance and thermal shock resistance of magnesia-carbon bricks are greatly affected by the raw materials, such as the quality of magnesia, particle distribution, and the selection of additives. Higher purity magnesia used in magnesia-carbon bricks, fewer B2O3 impurities, and a higher carbon-sulfur ratio result in better erosion resistance of the lining bricks. Magnesia-carbon brick slag lines made from fused magnesia with a carbon content controlled at around 14% exhibit better erosion resistance.
3. Modify the masonry process and optimize brick design. Whether building a new ladle or repairing one, pay close attention to the structural issues of the refractory lining. For example, the difference between flat and vertical masonry, misalignment at the junction of the new slag line and the slag line during minor repairs, and the treatment of the mortar between the working layer and the permanent layer during construction.
4. Control argon blowing and power supply. LF furnaces typically have three-phase electrodes. If the electrode positions are misaligned, the heat from the slag near the electrodes and the slag temperature will be too high, causing destructive erosion of the magnesia-carbon brick slag line.
5. Strengthen ladle operation control and red-brick turnover.
6. Add an anti-oxidation coating to the ladle lining. Some units do not perform anti-oxidation treatment on the carbon-containing working layer during the baking process after ladle construction, resulting in a tens of mm thick layer of oxidation and decarburization on the magnesia-carbon brick layer after baking. Therefore, the service life of magnesia-carbon bricks in the slag line area can be increased by adding an anti-oxidation coating.